GTAW
TG-S50
TIG welding rod and wire
Features: | - Good impact value at low temperatures
- Most widely used in japan
|
---|
Classification: | AWS A5.18 ER70S-G |
---|
Shielding gas: | Ar |
---|
Identification color: | 1st Yellow |
---|
Polarity: | DCEN |
Welding Positions:
Packaging data
| Spool | Tube |
φ mm | kg | kg | Length mm | g/piece |
0.8 | 10 | - | - | - | - |
1.0 | 10 | - | - | - | - |
1.2 | 10 | 20 | 5 | 1,000 | 9 |
1.6 | 10 | - | 5 | 1,000 | 16 |
2.0 | - | - | 5 | 1,000 | 25 |
2.4 | - | - | 5 | 1,000 | 35 |
3.2 | - | - | 5 | 1,000 | 63 |
Volume mm | 240W, 110H, 230L | 280W, 110H, 270L | 40W, 35H, 1015L |
Composition (wire mass%)
| Typical | Guarantya |
C | 0.10 | 0.02-0.12 |
Si | 0.74 | 0.40-0.95 |
Mn | 1.40 | 1.00-1.50 |
P | 0.011 | 0.025 |
S | 0.012 | 0.025 |
Cu | 0.24 | 0.50 |
Al | <0.01 | 0.15 |
Ti | <0.01 | 0.15 |
Zr | <0.01 | 0.12 |
Note: aSingle values are maximium. |
All-weld mechanical properties
| Typical | Guaranty |
0.2%YS (MPa) | 480 | 380 | 400min. |
TS (MPa) | 580 | 500 | 483min. |
EI on 4d (%) | 33 | 36 | 22min. |
IV -29°C (J) | 180 | 230 | 27min. |
PWHT (°Cxh) | AW | 625x8 | AW |
ABS | 3Y |
LR | 3Ym, H15
|
---|
DNV | ⅢYM |
BV | SA3YM |
---|
NK | KSW53G (I) |
CCS | 3, 3YSM |