SMAW
NC-39MoL
Stick electrode
Features: | - Suitable for dissimilar-metal joint and underlaying on ferritic steels
|
---|
Classification: | AWS A5.4 E309LMo-16 |
---|
Redrying Conditions: | 150~200℃x0.5~1h |
---|
Identification color: | 1st Silver, 2nd Blue |
---|
Polarity: | AC, DCEP |
Welding Positions:
Packaging data
φ mm | Length mm | kg/pack | kg/carton | g/piece | carton mm |
2.6 | 300 | 2 | 20 | 19 | 300W, 95H, 330L |
3.2 | 350 | 5 | 20 | 33 | 175W, 135H, 380L |
4.0 | 350 | 5 | 20 | 54 | 175W, 130H, 380L |
5.0 | 350 | 5 | 20 | 85 | 175W, 130H, 380L |
Composition (all-weld metal mass %)
| Typical (AC) | Guarantya |
C | 0.03 | 0.04 |
Si | 0.51 | 1.00 |
Mn | 1.3 | 0.5-2.5 |
P | 0.02 | 0.04 |
S | <0.01 | 0.03 |
Ni | 12.9 | 12.0-14.0 |
Cr | 23.5 | 22.0-25.0 |
Mo | 2.1 | 2.0-3.0 |
Cu | 0.07 | 0.75 |
Note: aSingle values are maximium. |
Welding parameters (A)
φ mm | 1F, 1G, 2F, 2G | 3G uphill, 4G |
2.6 | 50-85 | 45-80 |
3.2 | 70-115 | 65-110 |
4.0 | 95-145 | 85-135 |
5.0 | 135-180 | - |
All-weld mechanical properties
| Typical (AC) | Guaranty |
0.2%YS (MPa) | 450 | - |
TS (MPa) | 630 | 518min. |
EI on 4d (%) | 41 | 30min. |
IV 0°C (J) | 65 | - |